Cored Wires

(composition is nominal)

OSU 3501
Composition: Fe 4.7B 1.2Mn 1.5Si 1.0C
Coating hardness:  850 – 1000 HV10/0.1
Machining: Grinding
Properties: Friction resistant, highly erosion resistant
  Applications: Dust-conveying fans, screw conveyors, cyclone housings, storage bins, etc.
OSU 3502
Composition: Fe 17Cu 3Ti 1.3Si 1Mn
Coating hardness:  570 – 850 HV10/0.1
Machining: Grinding
Properties: Erosion and thermal shock resistant up to 600 °C (1100 °F)
  Applications: Steam lines, fluidized bed kiln components, power plant furnaces, protection for boiler components (ex. boiler tubes), steam turbine casings, high-temperature cyclones, exhaust gas fans
OSU 3509
Composition: Fe 28Cr 6Al 3Mo 0.2C
Coating hardness:  270 HV10/0.1
Machining: Grinding
Properties Erosion and corrosion resistant up to 900 °C (1650 °F)
Applications: Pulverized coal-fired boilers
OSU 3510
Composition: Fe 13Cr 1.2Mo 0.16C 1.0Si 1.0Mn
Coating hardness:  320 HV10/0.1
Machining: Grinding
Properties: Erosion and wear resistant
  Applications: Coatings for pulp and paper mills, mixer arms and blades, screw conveyors for pulp processing
OSU 3515
Composition: Fe 27Cr 2.7B, 1Si 0.8Mn 0.1C
Coating hardness:  500 – 600 HV10/0.1
Machining: Grinding
Properties: Erosion and corrosion resistant up to 200 °C (390 °F)
Applications: Dryer rollers for the paper manufacturing industry
OSU 3531
Composition: Ni 15Cr 5.0Si 1.9W 0.5B 0.04C
Coating hardness:  300 – 400 HV10/0.1
Machining: Grinding
Properties: High corrosion and wear resistance up to 200 °C (390 °F)
Applications: Barrel extruders, mould manufacture for fired materials
OSU 3535
Composition: Ni 50Cr
Coating hardness:  300 – 400 HV10/0.1
Machining: Grinding
  Properties: High temperature corrosion and oxidation resistance up to 800 °C (1475 °F)
Applications: Boilers in very sulfurous atmospheres
OSU 3550
Composition: Fe-based
Coating hardness:  3700 – 850 HV10/0.1
Machining: Grinding
  Properties: High temperature corrosion resistance up to 450 °C (840 °F)
Applications: Heat exchanger tubes, boiler walls for trash incineration
OSU 3560
Composition: Co 30Cr 12W 2.5C 2.3Ni 2.2Fe 1Si 1Mn
Coating hardness:  350-550 HV10/0.1
Machining: Grinding
Properties: High corrosion and wear resistance up to 900 °C (1745°F)
Applications: Barrel extruders, plastic mixers